Characterization of MITLL CCID20-W93c1 thin 2k x 4k pixel size 15um x 15um hz, new coating and laser annealing Reported by M.Wei Jul.9,1998 Both "R"(A) and "L"(B) amps worked TEST CONDITIONS temperature: -130c Voltages: Vdd = +19v Vr = +12.5v Vopg = 0v Vsub = 0v Vp1,2,3 = +2, -6v Vs1,2,3 = +6, -3v Vsw = +5, -5v RG = 10, 0v SCP = 10v read 3800(r)x2048(c) area only. changed gain of preamp. from 21 to 4.83 TEST RESULTS e-/DN: R: 0.40 Determined by Fe55 x-ray test L: 0.37 serial CTE R: 0.9999885 Determined by Fe55 x-ray test L: 0.9999958 Determined by Fe55 x-ray test vertical CTE 0.99999854 Determined by cosmic ray Vertical charge traps: 4 (in 2048(r) x 2048(c) area) Determined by charge-pumping method Read noise: R: 2.32e- DSC timing: 16us on data and 16us on baseline 2.44e- DSC timing: 4us on data and 4us on baseline L: 2.03e- DSC timing: 16us on data and 16us on baseline 2.15e- DSC timing: 4us on data and 4us on baseline Full well(nonmpp) 101 ke- Dark current: Measured from 1000s integration (nonmpp) 1.26e-/hour/pixel (@-130c) QE(%) -80c -90c -120c -130c 3200A 10.9 10.1 8.4 6.8 3500A 15.7 14.3 11.2 9.7 4000A 41.3 42.7 40.2 40.5 4500A 52.2 51.0 49.3 47.8 5000A 62.9 60.2 61.8 59.4 6000A 73.5 73.6 72.5 68.8 6500A 76.6 77.2 74.6 72.0 7000A 80.8 81.1 77.8 74.5 8000A 66.9 65.5 62.4 58.8 9000A 40.1 37.8 34.0 32.0 10000A 8.5 7.6 5.7 5.1 Fringing 8000A 13.5% 9000A 11.6% 10000A 15.6% --------------------------------------------- Spurious Charges(e-): from a 1 sec dark field vv=2,-6 vv=2,-8 top of CCD: 0.06 2.56 mid of CCD: 0.1 3.4 bottom of CCD 0.24 4.32 QE variations(%) - wavelength - temperature of w93c1 CCD w.l.(A) -130c -120c -90c -80c 3200 43.5 39.0 35.6 32.2 3500 46.8 44.3 36.6 34.5 4000 6.1 5.7 6.8 7.0 4500 2.6 1.7 3.0 3.5