Characterization of MITLL CCID20-W88c2 thin 2k x 4k pixel size 15um x 15um Laser annealing ?? new AR coating Reported by M.Wei Aug.14,1998 Both "R"(A) and "L"(B) amps work bad brick wall pattern (type 3) TEST CONDITIONS temperature: -130c Voltages: Vdd = +19v Vr = +12.5v Vopg = 0v Vsub = 0v Vp1,2,3 = +2, -6v Vs1,2,3 = +6, -3v Vsw = +5, -5v RG = 10, 0v SCP = 10v read 3800(r)x2048(c) area only. changed gain of preamp. from 21 to 4.83 TEST RESULTS e-/DN: R: 0.38 Determined by Fe55 x-ray test L: 0.41 serial CTE R: good Determined by Fe55 x-ray test L: 0.99998 Determined by Fe55 x-ray test vertical CTE very good Determined by Fe55 x-ray test Vertical charge traps: 3 (in 3800(r) x 2048(c) area) Determined by charge-pumping method Read noise: R: 1.8e- DSC timing: 16us on data and 16us on baseline 2.3e- DSC timing: 4us on data and 4us on baseline L: 1.9e- DSC timing: 16us on data and 16us on baseline 2.6e- DSC timing: 4us on data and 4us Full well(nonmpp) 104 ke- Dark current: (@-130c) 0.64e-/pixel/hour QE(%)(average of big area) w.l. -130c -85---90c 3200 6.8 15.8 3500 10.6 23.6 4000 24.9 45.2 4500 29.7 52.7 5000 34.4 63.2 6000 46.9 70.2 6500 54.6 73.1 7000 59.3 78.7 8000 51.2 65.7 9000 28.5 38.2 10000 4.7 8.1 Fringing 8000A 8.0% 9000A 8.0% 10000A 20.0% --------------------------------------------- QE variations of CCID20 w88c2 at -130c and -90c(%) wavelength -130c -85--90c 4000 99.3 12.3 4500 95.8 12.4 5000 96.4 13.0 6000 67.3 10.5 6500 48.5 8.1 7000 40.6 6.9 8000 27.5 4.8 9000 23.6 3.3 10000 16.7 0.0 QE variations - temperature of CCID20 w88c2(%) 4000A 6500A 9000A -130 99.3 48.5 23.6 -120 68.2 38.6 20.1 -110 50.0 31.5 18.1 -100 34.9 21.4 10.7 -90 14.0 11.0 5.7